Storage and Handling of Fluxes
Storage
- Unopened flux bags must be stored in maintained storage conditions as follows:
Temperature: 68°F, +/- 18°F (20°C, +/- 10°C)
Relative humidity: As low as possible - not exceeding 60% max. - Fluxes should not be stored longer than 3 years.
- The content of unheated flux hoppers must, after an 8 hours shift, be placed in a drying cabinet or heated ?ux hopper at a temperature of 300°F, +/- 45°F (150°C +/- 25°C).
- Remaining flux from unopened bags must be placed at a temperature of 300°F, +/- 45°F (150°C +/- 25°C).
Re-Cycling
- Moisture and oil must be removed from the compressed air used in the re-cycling system.
- Addition of new flux must be done with the proportion of at least one part new ?ux to one parts re-cycled ?ux.
- Foreign material, such as millscale and slag, must be removed by a suitable system, such as sieving or magnetic separator.
Re-Drying
- When handled and stored as above, the ESAB ?uxes can normally be used straight away.
- In severe applications, stipulated by the applicable material speci?cation, re-drying of the ?ux is recommended.
- Furthermore, if the flux has somehow picked up moisture, redrying can return the ?ux to its original moisture content.
- Re-drying shall be performed as follows:
Agglomerated ?uxes: 570°F, +/- 45°F (300°C +/- 25°C) for about 2-4 hours.
Fused ?uxes: 390°F, +/- 90°F (200°C +/- 50°C) for about 2-4 hours. - Re-drying must be done either in equipment that turns the flux so that the moisture can evaporate easily or in an oven on shallow plates with a flux height not exceeding 2 in (5 cm).
- Re-dried flux, not immediately used, must be stored at 300°F, +/- 45°F (150°C +/- 25°C) before use.
Disposal
- Discard any product, residue, disposable container or liner in an environmentally acceptable manner, in full compliance with federal and local regulations.
- Please address your local disposal company for prescribed disposal.
- Information on product and residues are given in the Safety Data Sheets available through www.esabna.com/msds.